Inconel 718 Wrought nickel-base superalloy
          
Inconel 718 Alloy is a nickel based superalloy , at -253 - 700 degree temperature range Inconel 718 Alloy steel has good comprehensive properties. The yield strength of Inconel 718 Alloy steel under 650 degree temperature is the best among all the Wrounght nickel-base superalloy With a good anti fatigue, anti radiation, antioxidation, corrosion resistance, and processability, good welding performance and long-term stability, to complexmanufacturing various shapes of parts, in the aerospace, nuclear,petroleum industry, in the temperature range is widely used.
1.Inconel 718 Wrounght nickel-base superalloy equal material : UNS NO7718, Nc19FeNb, , W.Nr.2.4668, NiCr19Fe19Nb5, NiCr19Nb5Mo3
2. Inconel 718 Wrounght nickel-base superalloy Chemical composition :
Inconel 718 Alloy steel chemical composition is divided into 3 categories: standard components, high quality components, high pure component,High quality components based on standard components of the carbon reduction and increase of niobium, thereby reducing the number of niobium carbide,reduce fatigue and increase the amount of strengthening phase, improve the anti fatigue performance and strength of materials. At the same time, reduce the harmful impurities and gas content. High pure components is to reduce the content of sulfur and harmful impurity in high quality standard basis, improve the comprehensive performance of the material purity .
Inconel 718 alloy steel for nuclear energy applications, control of boron content (other elements unchanged), specific content determined by both sides. In order to Distinguish with Inconel 718 alloy in aerospace industry, When (B) ≤ 0.002% in Inconel 718 alloy steel,we call it as alloy Inconel 718A
Inconel 718 standard components, high quality components, high pure component %
| 
				 
					Category  
			 | 
			
				 
					C 
			 | 
			
				 
					Cr 
			 | 
			
				 
					Ni 
			 | 
			
				 
					Co 
			 | 
			
				 
					Mo 
			 | 
			
				 
					Al 
			 | 
			
				 
					Ti 
			 | 
			
				 
					Fe 
			 | 
		|||||||
| 
				 
					Standard 
			 | 
			
				 
					≤0.08 
			 | 
			
				 
					17.0~21.0 
			 | 
			
				 
					50.0~55.0 
			 | 
			
				 
					≤1.0 
			 | 
			
				 
					2.80~3.30 
			 | 
			
				 
					0.30~0.70 
			 | 
			
				 
					0.75~1.15 
			 | 
			
				 
					remaining 
			 | 
		|||||||
| 
				 
					High quality 
			 | 
			
				 
					0.02~0.06 
			 | 
			
				 
					17.0~21.0 
			 | 
			
				 
					50.0~55.0 
			 | 
			
				 
					≤1.0  
			 | 
			
				 
					2.80~3.30 
			 | 
			
				 
					0.30~0.70 
			 | 
			
				 
					0.75~1.15 
			 | 
			
				 
					remaining 
			 | 
		|||||||
| 
				 
					High purity 
			 | 
			
				 
					0.02~0.06 
			 | 
			
				 
					17.0~21.0 
			 | 
			
				 
					50.0~55.0 
			 | 
			
				 
					≤1.0 
			 | 
			
				 
					2.80~3.30 
			 | 
			
				 
					0.30~0.70 
			 | 
			
				 
					0.75~1.15 
			 | 
			
				 
					remaining 
			 | 
		|||||||
| 
				 
					Category 
			 | 
			
				 
					Nb 
			 | 
			
				 
					B 
			 | 
			
				 
					Mg 
			 | 
			
				 
					Mn 
			 | 
			
				 
					Si 
			 | 
			
				 
					P 
			 | 
			
				 
					S 
			 | 
			
				 
					Cu 
			 | 
			
				 
					Ca 
			 | 
		||||||
| 
				 
					Not more than  
			 | 
		|||||||||||||||
| 
				 
					Standard 
			 | 
			
				 
					4.75~5.50 
			 | 
			
				 
					0.006 
			 | 
			
				 
					0.01 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.015 
			 | 
			
				 
					0.015 
			 | 
			
				 
					0.30 
			 | 
			
				 
					0.01 
			 | 
		||||||
| 
				 
					High quality 
			 | 
			
				 
					5.00~5.50 
			 | 
			
				 
					0.006 
			 | 
			
				 
					0.01 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.015 
			 | 
			
				 
					0.015 
			 | 
			
				 
					0.30 
			 | 
			
				 
					0.01 
			 | 
		||||||
| 
				 
					High purity 
			 | 
			
				 
					5.00~5.50 
			 | 
			
				 
					0.006 
			 | 
			
				 
					0.005 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.35 
			 | 
			
				 
					0.015 
			 | 
			
				 
					0.002 
			 | 
			
				 
					0.30 
			 | 
			
				 
					0.005 
			 | 
		||||||
| 
				 
					Category 
			 | 
			
				 
					Bi 
			 | 
			
				 
					Sn 
			 | 
			
				 
					Pb 
			 | 
			
				 
					Ag 
			 | 
			
				 
					Se 
			 | 
			
				 
					Te 
			 | 
			
				 
					Tl 
			 | 
			
				 
					N 
			 | 
			
				 
					O 
			 | 
		||||||
| 
				 
					Not more than  
			 | 
		|||||||||||||||
| 
				 
					Standard 
			 | 
			
				 
					--- 
			 | 
			
				 
					--- 
			 | 
			
				 
					0.0005 
			 | 
			
				 
					--- 
			 | 
			
				 
					0.0003 
			 | 
			
				 
					--- 
			 | 
			
				 
					--- 
			 | 
			
				 
					--- 
			 | 
			
				 
					--- 
			 | 
		||||||
| 
				 
					High quality 
			 | 
			
				 
					0.001 
			 | 
			
				 
					0.005 
			 | 
			
				 
					0.001 
			 | 
			
				 
					0.001 
			 | 
			
				 
					0.0003 
			 | 
			
				 
					--- 
			 | 
			
				 
					--- 
			 | 
			
				 
					0.01 
			 | 
			
				 
					0.01 
			 | 
		||||||
| 
				 
					High purity 
			 | 
			
				 
					0.00003 
			 | 
			
				 
					0.005 
			 | 
			
				 
					0.001 
			 | 
			
				 
					0.001 
			 | 
			
				 
					0.0003 
			 | 
			
				 
					0.00005 
			 | 
			
				 
					0.0001 
			 | 
			
				 
					0.01 
			 | 
			
				 
					0.005 
			 | 
		||||||
3. Inconel 718 Alloy steel property :
Inconel 718 Alloy melting temperature range : 260-1320 degree
Inconel718 Alloy Density: 8.24g/cm3.
4. Inconel 718 Specifications and supply status : We can supply forging parts (disc, the integral), cake, ring, bar (forging rod, bar, cold rolling, plate, wire rod), belt,tube, different shapes and sizes of fasteners, elastic components, delivery conditions agreed upon by both sides of supply and demand. Wire to the agreed delivery state into a disc delivery.
5.Inconel 718 alloy Application and specific requirements: Various pieces of a manufacturing and aerospace engines and rotating parts, such as disk, ring,casing, shaft, blades, fasteners, elastic element, gas conduit, sealing element and welding pieces of the structure; nuclear industrial applications of various elastic components and framework; application of manufacturing oil and chemical industry parts and other parts.Various pieces of a manufacturing and aerospace engines and rotating parts, such as disk, ring, casing, shaft, blades, fasteners, elastic element, gas conduit, sealing element and welding pieces of the structure; nuclear industrial applications of various elastic components and framework; application of manufacturing oil and chemical industry parts and other parts
Product
          - Nickle alloys & Super alloys
 - Stainless steel & Heat resistant steel
 - Carbon steel
 - Low alloy high strength steel
 - High strength steel
 - Boiler steel plate
 - Shipbuilding steel plate
 - Bridge structural steel
 - Weathering steel
 - Wear resistant steel
 - Pipeline steel
 - High carbon steel
 - Alloy steel
 - CQ/DQ/DDQ/CSS/HSS Grade steel
 - Hot rolled steel coil
 - Cold rolled steel coil
 - Pickled & oiled steel coil
 - Electrical steel
 - Galvanized and prepainted steel
 - Shipbuilding angle steel bar
 - Shipbuilding bulb flat bar
 - Shipbuilding L shape bars
 
About Us
          
           Manufacture
          
          
       